(1) Kiln discharge port and discharge belt: The lining materials used in these two places are subject to serious mechanical wear and chemical corrosion. Therefore, the lining materials used in these parts are required to have good abrasion resistance and resistance to sudden temperature changes. The discharge belt generally uses high-aluminum bricks with an Al2O3 content of 70% to 80%, thermal shock-resistant high-alumina bricks, spinel bricks and magnesia-chrome bricks; the discharge port uses high-alumina refractory bricks and corundum as aggregate. Heat-resistant concrete and sometimes silicon carbide bricks are used.
(2) Firing zone: Since the firing zone is calcined at high temperature and combined with spinel and periclase, it has higher cold and hot strength and better thermal shock stability. Generally, magnesia-chromium bricks and polyethylene bricks are used. Sodium phosphate bonded magnesia bricks, alkali-resistant bricks and other directly bonded magnesia-chromium bricks fired at high and ultra-high temperatures.

(3) Transition zone: This zone is adjacent to the firing zone. The temperature changes frequently, the temperature of the cylinder is high, the kiln skin hangs and falls off sometimes, and chemical corrosion is also serious. Commonly used refractory materials include high-alumina bricks made of corundum and bauxite with 50% to 80% Al2O3, direct bonded magnesia-chrome refractory bricks, ordinary magnesia-chrome bricks and spinel bricks.
(4) Cooling zone: The temperature in this zone is still relatively high, but the chemical erosion is not as serious as the previous zone. Magnesia-chrome bricks, high-alumina bricks, phosphate-bonded high-alumina bricks and magnesia-alumina spinel bricks are generally used.
(5) Decomposition zone: In the part of this zone connected to the preheating zone, due to the small thermal stress and chemical stress, clay bricks of various qualities, high alumina bricks, lightweight bricks calcined into chemical bonds or ordinary bricks can be used. Magnesia chrome bricks; in the high wear and high temperature area connected to the transition zone, high alumina bricks, ordinary magnesia chrome bricks or spinel bricks with an Al2O3 content of 50% to 60% can be used.
(6) Preheating belt: The lining material of this belt needs to have sufficient alkali resistance and heat insulation properties. Generally, alkali-resistant insulating clay refractory bricks are used. When using lightweight bricks, the kiln barrel temperature can be reduced by 60-100°C compared with clay bricks of the same thickness. For dry kilns, the unit heat consumption can be reduced by 21-38kJ/kg clinker.
(7) Preheater system: Generally, alkali-resistant clay bricks are used in the straight tube, cone parts and connecting pipes of the preheater and decomposition furnace, and are added with an insulating composite layer and built with fire mud; the top cover can be The ceiling is made of fire bricks, backed by mineral wool, or concrete can be cast; castables are often used in elbows everywhere; semi-siliceous clay bricks with dense structure are used in the rising pipes at the end of the kiln to prevent alkali erosion.
(8) Cooler system: The temperature of the material inside the grate cooler changes the most, and the fire bricks are eroded unevenly. It is generally believed that the corrosion is most severe at the cooling opening and between the air inlet of the tertiary air duct and the cooling shrinkage. In addition, since the accumulation of dust limits the expansion of the masonry itself, it will also cause overall damage to the side walls. The refractory materials used in the grate cooler system include refractory bricks, lightweight castables, insulation bricks, insulation boards, etc. Ordinary magnesia chrome bricks and high alumina bricks can be used in the blanking throat area and high temperature areas; clay bricks can be used in medium and low temperature areas.